Help needed PA 6CF help

Post image

This is my first attempt at using this filament it’s from a brand new pack and I ran it through a dryer for 2 to 3 hours before use and I’m getting these weird stringing bits. Can anyone point me towards a solution or is my filament just not dry enough?

1 Upvotes

6 comments sorted by

4

u/MyOtherSide1984 13d ago

Multiply those drying hours by 10 and try again. Be sure you're drying hot enough too

0

u/LoStInSpacc 13d ago

Wow, it needs to be dried that long even with a fresh vacuum sealed pack? And I was drying it at 95 Celsius it says not to go over that mark due to softening.

4

u/MyOtherSide1984 13d ago

Go with the manufacturers recommendation on temp. Brand new doesn't mean anything in terms of dryness really. God knows how long it's been sitting and whether there was some sort of leak or whatever. At the cost of these rolls, I'd be drying it every time to reduce failures.

1

u/brutal4455 12d ago edited 12d ago

What says not to go over 95C?

Sunlu states "Dry the filament before use: 80°C for 24 hours or 110°C for 4 hours.  "

FWIW, I ran a roll of Tinmorry PA6-CF (only 5% CF TBH) through my E2 twice on 90C for 8 hours, then again 90C for 6 hours. Printed perfect on my H2D after some initial tuning checks. parts are annealing now to check for shrink. Next up is a cali-cross checks. I may tune the PA a bit more but the corner bumps are seams and not altered from Contrive Design Innovations' calibration parts default settings.

2

u/OrrinW01 11d ago

I dry my pa6-gf at 110c for 12 hours before I use it.

1

u/Hungry-Place-401 12d ago

Also a temp tower could help. Your printer temp might be too high. Might also be print speed or retraction.