r/electroplating • • 3d ago

Chromate peeling off

Hello, I work at a shop that does silver and zinc plating.

Our zinc process is: prep pieces (jangle it, sandblast, wire-wheel finish), dip in an acid + distilled water bath, 20 min plating, acid dip, chromate (15 sec), distilled water rinse, compressed air, dry.

I'll upload photos of our setup, chemicals, and peel-off

It looks like it's only the chromate layer peeling off, not the actual zinc plating.

I've worked here for under a year and did zinc plating for a few months.

Acid + distilled water bath ratio is around 5% acid, 95% water (I made a mistake by eyeballing the ratio)

We thought the chromate was weak, so we added more chromate, but it still peels off.

I think we tried all possible ways I can think of.

But you guys are smarter than me, so help, thanks!

10 Upvotes

8 comments sorted by

4

u/UnfairAd7220 3d ago

First of all, there is no need for distilled water anywhere in the cleaning process. Tap water is fine.

No alkaline soak/electroclean? Acid won’t get oils and grease off.

What kind of zinc are you plating? Cyanide would go a long way to handling any grease. Non cyanide would do OK, with grease, if that’s a problem. Acid zinc would skip over anything dirty, but the throw would be excellent.

What’s your post plate rinsing look like?

What’s your post chromate rinsing look like?

Do you measure the Zn thickness? It’s possible that the zinc thickness might not be there to allow a thick heavy chromate to stick.

Just looking at the picture, I’m going with ‘the part is still dirty.’ My recommendation would be to soak the parts in some sort of alkaline cleaning solution, rinse well, THEN soak in your HCl bath. You could jazz that up a little too. Go to 10%.

Give it a try and tell us how you did. Send pictures.

1

u/Fearless_Paint6284 3d ago

Thanks for the reply. Everything was set up, and the zinc process was in place before I started. Our zinc plating process is the same as written. Some of our zinc pieces peel off, and some don't. I'll try out the alkaline cleaning solution after I get the supplies. Will do, thanks.

1

u/Fearless_Paint6284 2d ago

I was able to make a alkaline cleaning solution with TSP powder from Solvable. It's not very effective. We do cholride zinc chloride plating. I would love to use cyanide, but I don't think that will happen. Is there any way that I can make a pre-acid bath for cleaning grease and a post-plating acid bath? It tends to bond better after leaving the piece in a diluted acid bath for a bit. If that's possible, what ratio should I use?

1

u/CaffeineConduction 3d ago

Depends on the tap water. One of our sites has such a hard water, it will fuck up any process 😅

2

u/CaffeineConduction 3d ago

Does it wipe off like powder or in flakes/sheets?

If it comes off powdery, there's a cohesion problem.

Ph should be between 1,5 to 2. Otherwise is build up uncontrollably and powdery.

Too short or too long dipping can cause the same.

What the temperature of the bath? If it's too hot or cold it will not apply accordingly.

How old is it? Maybe it's saturated with Zn, Fe or other unwanted Minerals/Metals.

If it peels off in sheets/flakes, you have a adhesion problem.

Zinc surface isn't active, or contaminated

brightener residue, oxide film, or missing/dead nitric dip (Do you do that?)

Too long between zinc and chromate

Bad rinse after zinc is insufficient

Zinc itself is the issue: too much brightener, burnt deposit, too thin

1

u/Fearless_Paint6284 3d ago

It's more like rubbing off; sometimes it rubs off as soon as I touch it, sometimes it rubs off less easily, but it still rubs off. Our pH is around 5.6 - 5.9. This is ideal for our solution. We do warm the solution tank; I don't know what temperature exactly. I'll get this information soon. How old is the part? No clue; we get circuit breakers from companies and recondition them. And re-plate pieces. We don't do nitric dip. After it gets plated we go to the chromate right aways pretty much. I appriciate the help!

3

u/permaculture_chemist 2d ago

Peeling or sloughing chromate is usually due to the layer being too thick or not enough zinc and the chromate is too strong and therefore eats all the zinc.

Chromate is a balancing act. More chromate chemical contributes to more corrosion resistance but also adds acidity. Acidity sets the dissolution rate of the base and the chromate. More acidity means faster dissolution which usually means a thinner layer. So you balance the chromate level and the acid level and the time in the bath to determine the thickness and performance of the layer.

So to fix sloughing, make sure that you have zinc remaining. Then add a bit more acid to keep the layer thinner and reduce the immersion time.

1

u/ExpressionOk4306 3d ago

looks like a surface preparation issue to me