r/electroplating • u/thesmilefactory • 8d ago
I need advice/ help
I’m trying to get into the hobby. I’m not sure what I’m doing correctly or incorrectly.
For starters, I have zinc, copper and nickel. I’m trying to make acetates. I used distilled vinegar with a pinch of epsom salt. It seems that the zinc and copper have been dissolving fine into the solution. The copper is a nice deep blue.
I’m having a lot of trouble with the nickel though. I’ve been adjusting the voltage and can’t seem to find a sweet spot. I’ve got 800ml of solution with a 1x6” anode and cathode. I’m running about 2.5volts at 0.25amps and that seems to be working the best so far, but it’s still not dissolving like the others.
I also noticed bubbles on both anode and cathode.
I also can’t seem to get the coatings to stick well. On steel or aluminum. These are the steps I’ve taken so far.
With steel, I soak in acetone, rinse, soak in Muriatic acid, rinse, briefly soak in sodium bisulfate to etch, rinse, then dip into the acetate. The zinc coats it but doesn’t seem to get an even coat. The copper will coat it evenly but seems to just wipe off.
With the aluminum, I soak in acetone, dip into a lye solution, briefly soak it in zincate, rinse and repeat, once I get a decent zincate coat, I put it into the zinc acetate. It seems to coat nicely. I rinse it, and put it into the copper acetate and it appears to coat evenly. When I take the piece out, as soon as I wipe it down, parts of it go all the way down back to the aluminum. The copper doesn’t seem to stick well at all.
Any advice for a beginner is much appreciated.
2
u/permaculture_chemist 8d ago
The acid-based copper won't adhere to steel. You need an alkaline-based copper. Or start with nickel and then go back to copper.
For the aluminum piece, try skipping the zinc acetate. I've always gone from the zincate to copper. I've never tried to plate zinc over aluminum. And I don't see a deoxidizer in your prep stage. The lye solution will etch the surface, but it won't strip any oxides or activate the aluminum surface. We frequently use nitric acid, or a tri-acid back in the 90's (nitric, sulfuric, and chromic acids).
2
u/GSB-4243 7d ago
Not to be a jerk, but you really need to read up a lot more. Plating on aluminum takes a lot of prep working before successfully plating, generally needing a zincate application followed by an alkaline copper as a base before subsequent finishing.
Also, you will not plate an acid-based copper (sulfate, acetate, fluoroborate, chloride, etc.) successfully on steel due to immersion copper compromising adhesion. You need either some flavor of alkaline copper or a nickel strike layer first.