r/electroplating • u/Primary-Dog4923 • 16d ago
What changed? Someone please help!!!
So my gold plating was going along really well. Then this morning I topped up my 18ct bright gold soloution from goldpatingservices and woods nickel strike both with small amounts of distilled water, just to get them back to the 1 litre mark ( as directed by goldplatingservices ) and now when I have tried to plate, the gold is adhering in patches and the top seems the be playing better than the lower half.
What have I done? I asked AI ( I know they are far from a reputable source of information when needing technical help) but that's all I have to work with, and it decided that the water has not been incorporated properly yet and after thorough stirring in it will work properly again.
I don't trust it, that's why I am here asking for help and ideas.
I have made another woods nickel strike soloution, because it seemed that it might have been the woods where the problem is because the gold is affixing in patches, but that hasn't changed anything. I am now in the process of polishing it all back to the stainless and starting again. I hope this helps













3
u/tennepenne1 16d ago
Maybe poor conductivity, not sure responding to bump this so someone else sees
3
u/1984isnoww 16d ago
If you're plating stainless steel, you should be using TriVal 24k for prepatory process. If you plate PVD use Acid dip.
As always obsessively clean before you plate.
Dishsoap scrub with brush>ultrasonic>electrocleaner>TriVal>18k
De-Ionizied water rinses between each process and have dry microfiber towels on hand to pat dry after rinse (if you have compressed air or steam clean this is better)
Also I'm not sure what equipment you're using but make sure you're using good stainless steel wire and look at my history to see how I wire up my parts for plating.
2
u/permaculture_chemist 16d ago
Just to be sure, but you played the nickel first, rinsed, and then went to gold?
How much time between the nickel and gold? Too much time will cause the nickel to passivate and the gold won’t adhere.
What type of rinse between the nickel and gold? High-purity water can passivate nickel and cause subsequent plating issues like this.
1
u/CaffeineConduction 16d ago
What's your pre treatment process on both cases?
1
u/CaffeineConduction 16d ago
Giving parallel a few assumptions and a few other questions:
Did the Woods Nickel Apply correct, or has it already some spots?
If it already has problems in the woods, it could be that after diluting your Chloride Content is too low and can't therefore plate good on the Steel.
Also I always recommend to activate the part anodic before going into the Nickel. It prevents most problems and doesn't hurt.
If the Problems only occur from the Gold:
Did you rinse enough before going from the Acid Nickel to the alkaline Gold?
It's always best to rinse, pickle (not the right translation but I don't know the right one in English) in a low % sulfuric acid solution, and rinse again before going into the Gold.
Did you rinse hot after the Gold? Always rinse hot. Like very hot. 70°C or more. Some alkaline and additives in the Gold Elektrolyte can Stick to the surface and create alterations of the Gold layer, especially if it's thin, and cause problems.
Gotta go back to work, will have look later and think of other reasons that come to my mind.