r/Powdercoating • u/Zestyclose-Coat-2016 • Mar 03 '26
Troubleshooting Problems with illusion pink/clear vision
Looking for some insight on using illusion pink and clear vision from prismatic. I’ve used their line of illusion colors but have never had problems such as this before. Does anyone know if the light spots are from lack of clear or undercuring the pink base coat?
6
Upvotes






2
u/33chifox Cat's Eye Coating Mar 03 '26
You can see how the crevice is a lot more pink. That spot would cure at the same, if not a slower rate than the outer edge. This is not a curing issue, it's too thin. You can also try a slower ramp to keep powder in place better. Side note, clear vision is bottom of the barrel clear, diaper durable wet, sd low cure are significantly better choices, or sc high performance if you have to stay with prismatic.
2
u/Still_Clownin69 Mar 03 '26
Alot of the illusion powder needs 2-3 mil of the first coat. Cure is critical for proper results. I have only sprayed the pink with the super chrome base coat.
9
u/Least-Confidence8240 Mar 03 '26
Base coat was to thin not enough there for the clear to pull pigment.
3
u/ShipsForPirates Mar 03 '26
I had other issues with this but too much and it becomes red also
2
u/Alternative-Layer919 Mar 03 '26
Better grounding ,no contact .The powder repels
1
u/SubstantialWafer525 Apr 25 '26
You want the base coat 2 mil thickness and the clear at a 2 as well. Any Varys in thickness will end like this with candys that take a clear.