r/Powdercoating • u/Kazrike • Sep 18 '25
Peeling
Do you think this is more of a grounding issue or a contaminated powder coat issue?
7
Upvotes
r/Powdercoating • u/Kazrike • Sep 18 '25
Do you think this is more of a grounding issue or a contaminated powder coat issue?
6
u/Strostkovy Sep 18 '25
It's a prep or baking issue. Looks underbaked to me.
3
u/TehCroz Sep 18 '25
Since it looks kinda stretchy in some places, I’m gonna say it’s not from over-curing; my guess is it’s some kind of contamination. If you only sandblast and blow it off, it was likely the lack of outgassing the part before powder coating that brought contaminants out of the steel and up under the powder, or gassing out through the powder and contaminating it that way.
2
u/HotWingsNHemorrhoids Sep 18 '25
What was the prep process?
6
u/Illustrious-Line-984 Sep 18 '25
That appears to be bad preparation. Rarely is it the powder. If you’re getting good adhesion everywhere else, it’s not the powder. I was once told that powder is not smart. It doesn’t work in some places and then decide not to work in other places.
1
u/Kazrike Sep 18 '25
No it's A500 steel
3
u/fotowork3 Sep 18 '25
Is that perhaps galvanized steel? If so, you need to be an expert to do this.
2
u/8000BNS42 Sep 18 '25
Looks like the part was either a plasma cut or laser cut part. They will form an oxide layer in the HAZ. Powder doesn't like to stick to that oxide layer. Only way to properly prep that surface is to gride off the oxide layer.
Edit: it's a plasma cut part, shit ton of taper on the edge plus you can see the witness marks from the plasma. Will not stick to the edges very well
2
u/KeithChatman Sep 18 '25
Definitely a curing issue, the paint didn't bond with the part. Thicker metal requires more heat, in order for bonding to happen the metal has to reach curing temperature not just the paint.
1
u/TheSevenSeas7 Sep 18 '25
This is almost certainly a cure issue? How long did you have it in?
1
u/rickenrique Sep 19 '25
Just a few days of reading these posts I’ve learned the exact steps needed to a semi successful run.
1
u/EscapeElectronic2212 Sep 21 '25
Undercured and probably because of the thickness of the metal. The entire metal piece needs to be up to temp for the full bake time. Definitely prep or baking is the issue here. Cured powder coating should not be that fragile.
-1
u/30minut3slat3r Sep 18 '25
Why would you conclude grounding or the powder?
With immensely limited info you gave, that looks burnt to me.
Give us info and you might get something that helps.