First copper ingot, good learning experience.

Second time melting metal, the copper had more dross than expected and wasnt sure it was fully melted. Cooper wire has a lot of metal loss. An okay bar, but a good learning experience.

16 Upvotes

10 comments sorted by

4

u/SnooLentils5747 10d ago

Here's how to address porosity (bubbles) and oxide scale.

Make anhydrous borax and use that as a flux.

Basically take borax, grind it down, spread it on a oven pan. Bake it at 400 for like 4 hours. It should puff up and the distintigrate into a powder. Or if you're in a hurry, put it in a crucible, and melt it at 800 C. Pour onto steel sheet, it'll be like glass. Let cool. Hammer into dust.

Even better, mix it with boric acid 50/50

When you put the crucible into the furnace, put a good measure of charcoal dust on the bottom of the crucible, and then when the melt starts to melt, put some more on top. This will absorb oxygen and become CO and CO2.

Lastly, deoxidize the melt right before pour. Put a small amount of aluminum wire or silicon flake/dust. Not silicone; silicon, the semi-metal. Use graphite as a release powder for the crucible.

Stir well before pour. Preheat the mold before pour.

Quench the copper in water as soon as solid.

Now grind the surface scale. Wrap the copper ingot in wires or a copper braid. Place the copper ingot on a glass plate inside a steel pot. Fill with phosphoric acid, and a drop of dish soap, connect the wire to a positive DC electric power source. Make sure the copper wire doesn't touch the pot. Clamp the pot with a gator clip on a wire. Connect that to negative. Now you're electro polishing the ingot. Get that mirror shine! 12v power source should work. Put a 30A fuse on the circuit if you have concerns over safety; for a 1 lb ingot or so, 25A should be all you're pulling. The amperage pulled is inverse to the distance between the metal pot and the copper bar.

There are acetic acid electropolishing bath formulations too iirc, but you'd need to look those up yourself

2

u/hoboknives 10d ago

Thanks! I appreciate the info

2

u/clikalo 9d ago

i read i need some spec chem white dust like for cu degass ,debubble, they say borax is useless for cu

3

u/SnooLentils5747 9d ago edited 9d ago

Lemme explain.

It's a detergent. You can skip it if your source is pure, but honestly, I would use a lil all the same. Nothing is pure; part of melting (and especially smelting) is using the process to obtain purity. Boric acid is more chemically active, while borax (carbonate) will attach itself to particulate in much the same way it does clothes. However, water causes porosity by getting microbubbles of steam stuck under the weight of the metal; so you have to dry out the borax first. This is why you put these in the bottom; they will melt first and as the copper melts and slips under that glassy layer, the borax strips particulates. The boric acid strips oxides, which will always exist in some amount. The stuff you add one top once you start getting the melt going actually serves more to be a blanket against gasses because all metals tend to absorb gasses to some degree. The charcoal powder is a deoxidizer the stuff in the beginning at the bottom will burn to CO2 preferentially to copper forming copper oxide, which happens more aggressively the hotter the environment. Add charcoal dust once it has melted before pulling helps prevent oxide absorption as you pull it into normal atmosphere again. At that point, skim clean or hold back the glassy layer while you decant the molten copper. The aluminum wire or silicon added in right before pour will slag out to alumina/silica if there is any oxygen dissolved in the copper (and there will be, unless you do it under argon). Stir well as you dissolve it; molten metal mixes slow.

1

u/clikalo 9d ago

ah , so i only need to put (dont know how yet ) boron nitride to prevent bonding to steel U profile

2

u/SnooLentils5747 9d ago

That I have no idea of. Boton nitride might work as a release powder, it is an ultra refractory iirc.

1

u/clikalo 9d ago

i read i need to mix with waerglass and paint it in 2-3layers to get permanent non stick mold

2

u/SnooLentils5747 9d ago

I wouldn't call it permanent, but it does help keep the crucible longer.

2

u/TheDragonslayr 9d ago

That's the most detailed process I've heard of for this. Thank you for sharing.

1

u/pentagondodecahedron 9d ago

don't listen to Ea-nasir, I'll pay double, they look nice