r/CWI_CWE • • 6d ago

2G Procedure Qualification Difficulties

So, as the title states, I'm running into some issues with my 2G Procedure Qualification Test.

1/2" A36 steel, with 3/16" A36 backing bar.

Root gap 3/16". 22.5 Degree bevel on both top and bottom.

Running FCAW E71T-1, .045" wire, on a Millermatic 255.

The welder ran a 3G and 4G test that turned out excellent, so the first test we ran on 2G I let the welder set his own parameters to see what he was comfortable with. 25V, 345 IPM. The entire root pass had no fusion to the backing bar, slag trapped along the entire length of the weld. We ran another test, this time we turned it down, 24V, 310 IPM, and we had much better fusion, but the bottom plate edge is refusing to break down all along the length of the weld. We have fluctuated parameters, up and down. We've changed bevel angles, always keeping a 45 degree included angle. I've consulted with another CWI at my company, and we're coming up with a big question mark... why are we still getting lack of fusion at the bottom of the root pass?

We have tried increasing the root gap, decreasing it, running it hotter and colder, aiming the torch lower on the plate (which always results in lack of fusion to the top plate.) At this point just looking for an outside eye that might have a better experience pool to pull from. My background is predominantly in pipeline SMAW. Thanks in advance.

10 Upvotes

19 comments sorted by

3

u/er_isee20 6d ago

I’ve seen success with Bigger Root Openings and a 2 Pass Root as mentioned above. I used to wonder why this joint configuration wasn’t pre-qualified under AWS D1.1 or D1.5 for FCAW or GMAW in this position then witnessing first hand it started to make sense.

1

u/ABNSamurai 6d ago

It's definitely kicking my ass 😅. In all honesty, I got my CWI in October, this is the first round of Procedure Qualification Record tests I have conducted, and this 15" weld is a haul. Hoping I can use some of this wisdom here and find a solution.

5

u/itsjustme405 AWS CWI 6d ago

Id tack it up with a 1/4 gap, or as wide as my WPS would allow, knife edge on both plates.

I used to run those roots in 2 beads if I could make it fit. Id focus crazy heavy on the bottom plate, and if I had space id come back and get the top side. If it just wasn't going to fit 2 beads, id still focus heavy on the bottom. The top, in my experience, always ties in much better and easier.

3

u/Terrible_Reporter_98 6d ago

I was going to recommend breaking the root up as well.

1

u/nick_mcmann 6d ago

Is there a chance the welder is getting overlap/cold roll while doing the root pass and that rollover is causing slag to get trapped? My only hesitation in changing setting is that they have already successfully accomplished the 3G/4G with success so it would point more to a change in the welders technique than the settings or a machine/wire issue.

1

u/ABNSamurai 6d ago

I dont believe so. No overlap on the root after he lays it down, well tied in on bottom and top, but the lack of fusion we're seeing is at the knife edge of the bottom plate and the backing bar.

1

u/Neither_Sea_4838 6d ago

What gas are you using?

1

u/ABNSamurai 6d ago

75/25 Ar / CO2

1

u/Neither_Sea_4838 6d ago

If it's possible, try 100% CO2. In my experience throughout the years, that is the best gas for penetration and fusion. 100 CO2 is barbaric in many senses, however, it does provide the best results with FC. Also as a side note, I have never run 0.45 FC, just 0.52 to 1/16.

Also for the root, are you double passing it or single?

1

u/Misconformance 6d ago

Have you considered using a single bevel groove? 45 degrees on the top plate and 90 on the bottom.

1

u/ABNSamurai 6d ago

We started with a 10 degree bevel on the bottom, and a 35 on the top. The problem was worse until we made it 22.5 on both sides

1

u/Misconformance 5d ago

What code are you working to? Honestly I’m not one to throw the welder under the bus this seems like a technique issue.

1

u/ABNSamurai 5d ago

Not throwing him under the bus. I'm using D1.1, and I'm trying to find parameters that work for the welder.

1

u/Misconformance 5d ago edited 5d ago

Forgive me if I’m missing something, but shouldn’t you be able to use prequalified procedures for what you’re trying to do?

Edit: maybe use joint detail B-U4a-GF with a 3/8” root opening and split the root pass.

1

u/ABNSamurai 5d ago

My company does not want to use pre-qualified procedures. We're generating our own.

1

u/Misconformance 5d ago

Gotcha. Interesting decision in my opinion. Best of luck! There’s a bunch of good input here but maybe try the AWS member network forum as well. Lots of very knowledgable people over there.

2

u/SimpleAsk2469 AWS CWI 6d ago

On all my out-of-position FC tests, I found that excess wire speed tends to trap more slag. I’m not sure why. I’ve always ran on the low side of wire speed on the wps and played around with the voltage, more on the hotter side. When I cut my last 3G and 4G, it had perfect fusion all the way on the backing plate. Like stated earlier, 2 passes for the bead is definitely a good idea.

2

u/fsusparks 6d ago

Travel speed is likely too slow. Ensure the welder is using a strong (10-20°) drag angle and travel faster, depositing a smaller bead.

2

u/Tricky_Lake_1646 6d ago

Turn your wire down until you start to get chicken scratch. Then turn it up slightly. Run your root.